An aluminum casting standards map matters because four regional systems describe the same metal in four different ways. ASTM B85 grades by chemistry plus a test bar, EN 1706 pairs an AC-4xxxx designation with a property class, JIS H 5302 uses ADC numbers, and GB/T 15115 uses YZ grades. The working cross-reference is ADC12 = A383 = EN AC-46100 = YL113. Treat those as chemically equivalent, not identical in tolerance or inspection, and cite both the alloy and the test standard in the purchase order.
关键要点
- Four documents govern one aluminum purchase: ASTM B85, EN 1706, JIS H 5302 and GB/T 15115. They agree on the middle of the range, not the edges.
- ADC12, A383, AC-46100 and YL113 share a chemistry family, but their silicon and copper windows differ by up to one percentage point.
- Mechanical values are comparable only when the specimen type matches. A cast-on bar and a separately cast bar give different numbers from the same heat.
- ASTM B85 sets no general dimensional tolerance. ISO 8062-3 and GB/T 6414 do, so the drawing must carry the CT grade.
- Radiographic acceptance is written as a severity level, not an adjective. ASTM E505 and ISO film practice number those levels differently.
- Naming the alloy and the inspection standard together removes the grey area that suppliers otherwise price into a quotation.
The Four Systems and What Each One Actually Controls
Each standard answers a different question, which is why a single drawing can be “compliant” in one country and out of specification in another. Reading them side by side shows where the overlap is real and where it is only assumed.
ASTM B85/B85M governs aluminum-alloy 压铸s in North America. It lists chemistry limits per grade in one table and tensile requirements in another, with the specimen taken from separately cast test bars. The grade name is a three or four digit number preceded by A, such as A380.0 or A413.0. The decimal place signals a die casting grade rather than an ingot grade.
EN 1706 is the European harmonized document. It designates each alloy as AC-4xxxx, for example AC-46000, and attaches property classes such as F, T5 and T6. Tensile values step down as the section thickness rises, because a thick section cools more slowly. That dependence is easy to miss when a European data sheet sits next to an ASTM table.
JIS H 5302 is the Japanese die casting standard and the one most Asian foundries quote by habit. Its ADC numbering (ADC1, ADC3, ADC10, ADC12, ADC14) is a chemistry-first system with a short mechanical table. Because the grade list is short and the numbers are memorable, ADC12 became the default shorthand for die-cast aluminum across China, Taiwan, Vietnam and much of Southeast Asia, even where the governing contract is ASTM.
GB/T 15115 is the Chinese die casting standard. Grades appear as YZAlSi11Cu3 and similar, shortened on the shop floor to YL numbers. A parallel document, GB/T 1173, covers gravity and 砂铸造 alloys under ZL designations, which is where A356-type heat-treatable grades appear. Both are national standards, both are widely cited in Chinese contracts, and neither is automatically accepted by a European notified body.
According to the North American Die Casting Association, product standards only work when the alloy, the test method and the acceptance level travel together in one document. That sentence is the whole exercise in a line: an alloy name alone proves almost nothing at the receiving inspection bench. A aluminum casting standards map is that idea applied across four regions at once.
Cross-Reference Table for the Grades Buyers Actually Buy
This aluminum casting standards cross-reference maps the six grade families behind most die-cast aluminum sourced from Asia. Read the last column first: it tells you which of the other four you need.
| Grade family | ASTM B85 | EN 1706 | 吉斯 H 5302 | GB die cast | 典型用途 |
|---|---|---|---|---|---|
| High-fluidity, thin wall | A383.0 | AC-46100 (AlSi11Cu2(Fe)) | ADC12 | YL113 / YZAlSi11Cu3 | Motor end covers, LED housings, electronic enclosures |
| General purpose, workhorse | A380.0 | AC-46000 (AlSi9Cu3(Fe)) | ADC10 | YL104 / YZAlSi9Cu3 | Pump bodies, brackets, general industrial castings |
| Corrosion resistance first | A360.0 | AC-43000 (AlSi10Mg) | ADC3 | YL104 with Mg addition | Outdoor enclosures, marine-adjacent hardware |
| Pressure tightness, low copper | A413.0 | AC-44100 (AlSi12(Fe)) | ADC1 | YL102 / YZAlSi12 | Leak-tested housings, thin-wall covers |
| Wear resistance, hypereutectic | A390.0 | No exact AC code (AlSi17Cu4Mg class) | ADC14 | YL117 | Compressor swash plates, wear faces |
| Heat-treated structural | A356.0-T6 (B108) | AC-42100 (AlSi7Mg0.3) | AC4CH (H 5202) | ZL101A / GB/T 1173 | LPDC and gravity structural parts, not HPDC |
Two warnings belong under that table. The last row is not interchangeable with the rows above it: A356-type alloys are gravity and low-pressure grades, and running them in a high-pressure cell produces hot tears and soldering. Also, “equivalent” means the chemistry bands overlap, not that the two standards are the same document. A supplier who quotes A380 and ships ADC12 ships a different alloy, even though both cast well.
Where the mapping is exact in practice, it is exact because the chemistry windows were written from the same parent specification. YL113 and ADC12 are the clearest case: silicon around 11 percent, copper around 2 to 3 percent, iron held under about 1 percent for die casting. That family is the default for aluminum motor end covers and thin-wall lighting bodies across Asia, and it is what most buyers receive when they ask for A383.

Where the Cross-Reference Breaks Down
Most rejections at goods-in are not caused by a bad casting. They are caused by a document pair that was never compatible, and the aluminum casting standards gap only appears when the certificate is compared with the purchase order line by line.
Chemistry windows are not the same width
ADC12 allows silicon from 9.6 to 12.0 percent and copper from 1.5 to 3.5 percent. A383 allows roughly 9.5 to 11.5 percent silicon and 2.0 to 3.0 percent copper. A heat running at 11.8 percent silicon and 3.4 percent copper passes JIS and fails ASTM on both counts. Nothing about the casting changed. The melt simply sits in the corner of one window and outside the other.
The same trap applies to iron. Each standard sets a different ceiling, and recycled feedstock drifts upward in iron run after run. That drift is why chemistry control at the furnace, not at the shipping dock, is the only place the problem closes.
Test bars are not the part
ASTM tensile values come from separately cast bars poured from the same melt. Those bars freeze slowly and cleanly, so they represent the best case for that chemistry. A 2 mm cover wall in the same heat freezes in under a second and carries far more porosity. A certificate showing 290 MPa does not promise 290 MPa in the wall the customer cares about.
Tolerance lives outside the alloy standard
ASTM B85 does not set a general dimensional tolerance table. ISO 8062-3 does, through CT grades that scale with nominal size, and ISO 8062-3 also distinguishes machined from as-cast features. GB/T 6414 mirrors the same CT logic in China. A drawing that cites only an alloy leaves tolerance undefined, and undefined tolerance at goods-in always resolves in favor of whoever wrote the inspection report.
Inspection severity is a number, not a word
Radiographic acceptance is the most negotiated line in any die casting contract. ASTM E505 grades discontinuities by severity level for a given thickness; ISO film practice and Chinese GB/T 11346 use their own scales. “No visible porosity” is not an acceptance criterion, because every die casting contains some. The buyer who writes “E505 level 2 in the bearing boss area” gets a measurable answer.
Mapping the Evidence: Which Test Standard Proves What
Alloy chemistry, tensile strength, hardness, dimensions, internal soundness and coating durability each need their own test document. A complete aluminum casting standards package names one standard per characteristic, and every one of those names should appear on the certificate you receive.
| 特征 | ASTM | ISO / EN | JIS | GB |
|---|---|---|---|---|
| 化学成分 | B85 / B108 | EN 1676, EN 1706 | H 5302 | GB/T 15115 |
| Tensile properties | E8/E8M, B557 | ISO 6892-1 | Z 2241 | GB/T 228.1 |
| Brinell hardness | E10 | ISO 6506-1 | Z 2243 | GB/T 231.1 |
| Dimensional tolerance | Drawing only | ISO 8062-3 | B 0403 | GB/T 6414 |
| Radiographic inspection | E505 | ISO 5579 | H 0521 | GB/T 11346 |
| Penetrant inspection | E165 | ISO 3452-1 | Z 2343-1 | GB/T 9443 |
| Salt spray resistance | B117 | ISO 9227 | Z 2371 | GB/T 10125 |
The blank cells are the interesting ones. Where a system has no direct equivalent, a supplier cannot simply “certify to the other standard” without a written deviation. Dimensional tolerance is the clearest example: there is no ASTM general tolerance table for die castings, so an American drawing without a tolerance block has no default. Ask for the CT grade and the feature list it applies to.
Salt spray is the second common gap. ASTM B117 and ISO 9227 run the same fog at the same concentration, but the pass criterion comes from the customer, not the standard. A 480-hour requirement means nothing until someone states whether the limit is red rust, white rust or adhesion loss. Write the criterion next to the hours.
How HKX Builds a Dual-Standard Inspection Plan
Most drawings that reach HKX cite one standard and imply another: a part number in AC-46100 arrives with an inspection sheet written in ASTM E505 language. HKX resolves that in a written plan before the first shot, and the plan travels with the job through the shop.
Chemistry is confirmed before the melt is released. A sample from each furnace charge goes to the direct reading spectrometer, and the result is checked against the tighter of the two applicable windows. For an ADC12 job with an A383 certificate requirement, that means holding silicon at or below 11.5 percent and copper inside 2.0 to 3.0 percent, not simply inside the broader JIS band. Modifier additions are logged against the charge number so the heat stays traceable to the ingot lot.
Dimensional work starts from a written datum scheme rather than the operator’s judgment. HKX establishes A-B-C datums on the machined mounting face and two bores, then runs a first article layout across every toleranced feature. The report lists nominal, tolerance, measured value and the CT grade applied to each as-cast dimension.
Internal soundness is sampled, not promised. X-ray coverage is set as a percentage of first-off parts plus a fixed production sampling rate, with acceptance stated as an ASTM E505 severity level in agreed zones. Pressure-tight parts get a pressure decay test with a recorded limit, and coated parts go to the salt spray cabinet on a defined schedule. Results land in a first article report, a material certificate with heat numbers, and a dimensional layout that match the standards on the drawing.

Which Standard Should You Specify?
The aluminum casting standards you name should be the ones your own quality system can audit. A US Tier 2 automotive buyer with PPAP obligations will find ASTM B85 easier to defend than a translated GB document. A European industrial buyer with a notified body in the loop needs EN 1706 and EN 10204 documentation. There is no universal right answer, only a right answer per supply chain.
Match the standard to the receiving inspection
Write what your incoming inspector can actually measure. Chemistry and tensile data arrive as paper, dimensions arrive as a CMM report, internal soundness arrives as film or a leak test record. If your lab cannot run a tensile test, a tensile requirement becomes a supplier self-declaration, which is weaker evidence than a hardness check you perform yourself.
Name the alloy twice
Put the customer-facing designation first and the supplier-side equivalent in brackets. “A383.0 (ADC12 or YL113 permitted)” removes ambiguity without forcing a Chinese foundry to translate its melt shop language. This line prevents most certificate disputes.
Keep a translation table in the contract
Attach the cross-reference as an appendix and state which document wins when they conflict. The default should be the stricter window, because that is the only rule a supplier cannot argue with at goods-in. For a deeper look at how Chinese grade names map to international ones, the guide to Chinese alloy grades covers the naming history behind YL and ZL.
Writing a Purchase Order That Survives an Audit
A purchase order is the only document that binds a foundry to a standard. Drawings get revised, emails get lost, and the certificate that ships references whatever the supplier decided to test. Six lines in the PO close that gap, and each one maps to a question an auditor will ask.
- Alloy designation, both systems. Primary designation plus the permitted equivalent, with the stricter chemistry window named.
- Test method per characteristic. Chemistry, tensile, hardness, radiography, leak and coating each get their own standard number.
- Acceptance levels, in numbers. E505 severity and zone, CT grade, leak rate limit, salt spray hours plus failure criterion.
- Sampling plan. First-off quantity, production frequency, and who pays for destructive tests.
- Documentation set. Material certificate with heat number, dimensional layout, first article report, and coating thickness records.
- Traceability rule. How the heat number is marked on the part or the packaging, and how long records are retained.
Two of those lines deserve expansion. Name the certificate type, because a mill test report to EN 10204 3.1 carries different weight than an in-house chemistry printout, and the difference is explained in this guide to reading a mill test report. State whether the heat number is stamped, laser marked or printed on the carton label, since a bag of unmarked parts cannot be traced after assembly.
The commercial logic is simple. A supplier who has to certify to a named method prices the inspection into the quotation, and that price is visible. A supplier working from an implied standard prices the risk instead, and the risk surfaces later as a rejected lot or a line stoppage. Buyers who write the six lines above pay for inspection once, and the aluminum casting standards they cite become enforceable instead of aspirational. The same discipline applies across a whole 铝压铸 program, not just the first part number.

经常问的问题
ADC12 和 A380 是同一款吗?
No. ADC12 sits closer to A383 on both silicon and copper. A380 allows about 3 to 4 percent copper and 7.5 to 9.5 percent silicon, while ADC12 allows 1.5 to 3.5 percent copper and 9.6 to 12 percent silicon. They behave similarly in a die, but a certificate for one does not satisfy the other.
Can a Chinese foundry certify to ASTM instead of GB?
Yes, and most exporters do. The alloy is melted to whichever window the contract names, and the report is issued against the ASTM method. What changes is the paperwork and the sampling discipline, not the metal. Confirm in writing which of the two aluminum casting standards governs the lot.
Why does my European drawing use AC-4xxxx codes instead of alloy names?
EN 1706 replaced national grade names with a single designation system so one code works across member states. The AC prefix means casting alloy, and the five digits encode the chemistry family. Property class letters such as T5 or T6 follow the designation.
What is the difference between GB/T 15115 and GB/T 1173?
GB/T 15115 covers die casting alloys, the ADC12 family poured into steel dies. GB/T 1173 covers gravity and sand casting alloys, the A356 family poured into permanent or sand molds. They are not interchangeable, and a ZL grade cannot be substituted into a high-pressure die.
How do I specify radiographic acceptance without slowing the program?
Name the standard, the severity level and the zones in one line, and agree on the sampling rate. Most programs settle on a tighter level in critical machined areas and a looser level elsewhere. That split keeps film review practical while protecting the features that actually carry load or seal.
Do these standards cover heat treatment tempers?
Partly. EN 1706 attaches property classes to tempers. ASTM handles tempers through separate specifications. For castings, the temper must be written on the drawing along with the property values expected after treatment.
作者:HKX 工程团队
HKX — 宁波合信模具有限公司,一家铝压铸件 中国宁波的制造商,拥有 30 多年的工具 经验,内部加工和精加工,ISO 9001和IATF 16949认证,以及20多个国家的客户。
与 HKX 工程团队交谈
Send a drawing and the standard it cites, and HKX will return a written inspection plan before quotation: the alloy window actually used at the furnace, the CT grade per feature, the radiographic severity and zones, the leak test limit, and the document set that ships with the lot. Buyers who bring an aluminum casting standards question usually leave with a one-page cross-reference they can attach to their own purchase order. To start that review, contact our engineering team with the drawing, the annual volume, and the certificate type your quality system requires.