The short answer is 0.5 mm of stock on a well-controlled die casting face. Where draft, warp or a parting line adds variation, 0.8–1.0 mm. On any high-pressure die cast feature, no more than 1.5 mm. Extra stock does not buy accuracy. It buys cycle time, tool wear and a better chance of opening porosity. Every machining allowance casting decision starts with the face being cut, not with the alloy or the tonnage.
Key Takeaways
- 0.5 mm per side covers a stable as-cast face; 1.0 mm covers a face that crosses the parting line or sits on a slide.
- Treat machining allowance casting numbers as arithmetic: stack variation, flatness, fixture repeatability and a cleanup margin.
- Draft tilts a wall, so stock measured normal to the surface is not the same at the top and bottom of the same face.
- Cutting deeper than about 1.5 mm removes the dense skin layer and exposes gas porosity that was never a problem before.
- Boring needs 0.2–0.3 mm radial stock; tapping needs a cored hole at tap drill size plus 0.1 mm, not stock.
- Two-sided stock callouts are the most common drawing error, because both faces share one wall.
The Three-Way Trade Behind Every Allowance
An allowance is a buffer between what the die produces and what the drawing needs. Too little and the cutter skips across a low spot, leaving a black patch where the as-cast skin survives. Too much and the shop pays for metal removal twice: once when the casting is poured, and again when the chips go in the bin. The correct number sits between those failures and is narrower than most drawings suggest.
Build the number instead of guessing it. Add four quantities: the casting tolerance on the face, the flatness or warp across it, the repeatability of the fixture that holds it, and a cleanup margin. A face held to ±0.15 mm with 0.15 mm of warp, on a fixture that repeats within 0.05 mm, already consumes 0.35 mm before any margin. Add 0.15 mm for cleanup and the honest allowance is 0.5 mm, not 2 mm.
That arithmetic is why machining allowance casting tables in old handbooks look generous. Many were written for sand and gravity castings, where variation is measured in millimeters rather than tenths. Carrying a 3 mm allowance onto a high-pressure die casting adds cost without adding capability. The die was never the source of the error that allowance was meant to absorb. According to the North American Die Casting Association, as-cast tolerance follows part size, so allowance should follow the same curve rather than a fixed habit.
Allowance is also directional. It is measured normal to the surface being cut, at the point where the tool enters, and before draft is applied. A note that says “0.5 mm stock” on a drafted wall is ambiguous unless the drawing states which end of the wall the dimension refers to. Shops resolve that ambiguity by leaving more, which is how a 0.5 mm intent becomes 1.2 mm of cut.
Stock Allowance by Face Type
In machining allowance casting, face type matters more than part size. A die casting has three kinds of surface, and each carries a different error budget. There are surfaces in one die half, surfaces that cross the parting line, and surfaces formed by a slide or core pin. The table below is the allowance schedule used for production quoting, expressed per side on the surface being machined.
| Face type | Stock per side | Why it needs that much | Risk if exceeded |
|---|---|---|---|
| Flat face in one die half | 0.5 mm | Position error only, no mismatch | Deep cut exposes porosity |
| Face crossing the parting line | 0.8–1.0 mm | Mismatch 0.05–0.10 mm plus flash | Longer cycle, more burr at the edge |
| Face on a slide or core pin | 1.0–1.5 mm | Slide clearance and wear add 0.1–0.2 mm | Ejector side becomes weak |
| Sealing face for an O-ring | 0.4–0.6 mm | Needs a fine finish, not a deep cut | Groove depth control is lost |
| Bearing bore, on diameter | 0.4–0.6 mm | Draft and core shrinkage | Bore runs off center in the boss |
| Bolt boss top face | 0.5–0.8 mm | Boss height varies with shrink | Boss shortens below clamp length |
| Thin wall under 2 mm | 0.3–0.5 mm | Little material to spare | Wall thins below design minimum |
| Large flat over 200 mm | 1.0–1.5 mm | Warp dominates the error budget | Cut is interrupted, poor finish |
Read the table as a starting point, not a rule. The thin-wall row is the one that catches designers. A 1.8 mm wall with 2 mm of stock on one side no longer exists as a wall. The machined result will be 0.5 mm thick in places. Where a wall must be machined, thicken the casting locally rather than relying on stock drawn from the wall. Check the design against the minimum wall thickness rules before the model is frozen.

Draft, Distortion and Clamping Eat the Allowance
Three effects quietly consume machining allowance casting stock before the tool touches the part, and none of them appear in a simple table.
Draft tilts the wall
A die casting needs draft to release, typically 1–2° on an outside wall and 2–3° on an inside wall. On a 50 mm tall wall, 1.5° of draft moves the surface by about 1.3 mm from bottom to top. If the allowance is dimensioned at the top, the bottom has 1.3 mm less; if it is dimensioned at the bottom, the top has more. Either way the cutter sees a tapered cut, and the finish pass has to follow the wall or leave a step.
Warp arrives after ejection
A 200 mm open frame will move 0.2–0.5 mm after it leaves the die. The movement continues for hours as the part equalizes. A casting measured hot on the bench and a casting measured the next morning are not the same part. Heat treatment makes it worse: a T6 cycle on a gravity casting can add another 0.3 mm of distortion, which is why quench fixtures exist.
Clamping pushes the part around
Any fixture applies force, and a thin-walled casting deflects under it. Over-clamp a 2 mm floor by 0.2 mm and the machined face springs back. It no longer matches the surface the probe measured in the fixture. Three-point support with light clamps at the stiffest bosses beats six clamps torqued to the limit, and the difference is often larger than the allowance itself.

What Excess Stock Costs in Cycle Time and Porosity
Extra stock feels safe because it protects against a missed cleanup. It is not free, and the machining allowance casting budget pays the bill in three places.
Cycle time scales with volume removed
Roughing 1 mm instead of 0.5 mm off a 100 × 100 mm face removes twice the volume. At aluminum cutting rates that is roughly 27 g of chips instead of 13 g. On a face mill limited by horsepower per cubic centimeter, the pass also takes proportionally longer. Multiply by four faces on a housing at 50,000 parts a year and the extra stock becomes a permanent tax on every unit. The same arithmetic sits behind CNC machining cost models, where volume removed is the first variable.
Deep cuts open porosity
The as-cast skin of an HPDC part is dense for roughly 0.3–0.8 mm. That skin is the reason a casting can hold pressure at all. Cut 1.5 mm and the tool reaches the zone where gas porosity lives. Pores that were sealed become leak paths, cosmetic pits or thread failures. This is the strongest argument against generous allowances: the material being removed is often the best material in the part.
Tool life and residual stress
Interrupted cuts across a rough as-cast surface shock the insert, and a deeper cut means more inserts consumed per part. Removing a heavy layer also releases residual stress unevenly, so a face machined flat can bow after the fixture opens. Both effects are worse on thin, open geometry, and both disappear when the allowance is sized to reality rather than to fear.
Allowance by Machining Operation
The machining allowance casting number has to match the operation that consumes it. A boring bar and a tap need completely different starting conditions. Giving both the same blanket stock is how parts get scrapped at the second operation.
| Operation | Stock to leave | Result after machining | Notes |
|---|---|---|---|
| Face milling, single pass | 0.3–0.5 mm | Ra 1.6–3.2 µm, flat 0.05 mm | Best option on a stable as-cast face |
| Face milling, rough plus finish | 0.6–0.8 mm total | Ra 0.8–1.6 µm, flat 0.03 mm | Required where the face carries a seal |
| Boring a bearing seat | 0.4–0.6 mm on diameter | ±0.02 mm, Ra 0.8 µm | Leave 0.1 mm for the finish pass only |
| Reaming a dowel hole | 0.15–0.25 mm on diameter | H7 tolerance | Cast or drill undersize, never ream from as-cast |
| Tapping M6 | No stock, core hole 5.0 mm | 6H thread | Core at tap drill plus 0.1 mm; stock causes tap breakage |
| Drilling from a cored hole | 1.0–2.0 mm on diameter | Depends on drill size | Cored hole must be smaller than the drill, never larger |
| Spotfacing a boss | 0.5 mm | Flat 0.05 mm over the washer face | Interrupted cut, use a coarse pitch insert |
| Sawing off a gate stub | 1.5–2.0 mm | Rough sawn face | Follow with a face pass if the surface is functional |
The tapping row is the one that causes the most damage. Casting a hole with stock for a tap means the tap has to remove metal on three sides at once. In a 5 mm hole that is enough to snap it. Core the hole at tap drill diameter plus a tenth of a millimeter, and let the tap cut threads rather than clear a path.

How HKX Sets Allowance Before the Die Is Cut
At the Ningbo plant, the machining allowance casting schedule is agreed at the DFM stage and written into the die drawing, because stock added after the die exists means welding and re-cutting steel. The starting point is a face-by-face review against the parting line. Any surface that crosses the split gets 1.0 mm; surfaces inside one half get 0.5 mm; slides get 1.2 mm because slide clearance moves with wear.
The review then checks the thermal side. HKX holds the fixed half at 200–240 °C and the moving half at 220–260 °C, with separate circuits on deep bosses. An uneven die face produces an uneven part, and an uneven part spends allowance budgeted for something else. Vacuum valve timing is set so the cavity is evacuated 0.4 s before the shot and sealed within about 20 ms of fill. A cleaner cavity means less gas porosity just below the skin, which is exactly the depth a machining cut reaches. Before the die is accepted, HKX sections one casting through the heaviest machined face and measures the dense skin against the planned depth of cut. First-off parts go to CMM on three cast datum pads, and the as-cast report is compared with the model before a machining program is proven. If a face shows less than 0.3 mm of cleanup margin at the low corner, the die is corrected then, not after 20,000 parts.
The same review sets the fixture. Three-point support on machined bosses, clamps over the stiffest ribs, and a torque value written on the setup sheet. Air decay testing at 0.5 bar with a 0.3 mbar per minute limit follows machining on sealed housings. A pore opened by a deep cut is caught at the station rather than at the customer.
Writing Allowance Into the Drawing and the RFQ
Most allowance disputes start with a drawing note that cannot be measured. “Leave 1 mm for machining” is not a specification, because it does not say which surfaces, on which side, measured from where. A supplier that wants to be safe will take 1 mm everywhere, and the buyer pays for it in cycle time without knowing.
Write three things instead. First, mark the machined surfaces on the model and state stock per side for each group. A machining allowance casting schedule grouped by face type is what a shop can actually execute. Second, name the datum that the stock is measured from, so the allowance is not consumed by a datum shift. Third, state the finish and flatness required after machining, since that requirement decides whether one pass or two are needed. Reference the general cast tolerance as a class, such as ISO 8062-3 CT6, and call the alloy to ASTM B85/B85M, so the allowance and the as-cast band come from the same specification.
Two rules prevent the classic errors. Never dimension stock on both faces of one wall, because the two callouts share a single thickness and the shop will take the larger. And never specify allowance without a minimum remaining wall, because stock is drawn from the casting, not added to it. A 2 mm wall with 1.5 mm removed on one side is no longer a 2 mm wall.
In the RFQ, ask for the as-cast condition to be reported before machining starts. A supplier that measures the casting and reports the low-corner margin is managing the allowance; one that machines first and reports scrap later is discovering it. That single deliverable, an as-cast dimensional report with the stock actually available at each machined face, is worth more than any tolerance note on the drawing. It is also the document that settles the argument about who pays when a face does not clean up.
Frequently Asked Questions
How much machining allowance should I leave on a die casting?
A machining allowance casting schedule follows the face, not the alloy. Leave 0.5 mm per side on a flat face inside one die half, 0.8–1.0 mm where the face crosses the parting line, and 1.0–1.5 mm on a slide face. Anything above 1.5 mm on an HPDC part adds cost and porosity risk without improving the result.
Is 2 mm of stock too much?
For high-pressure die casting, yes. A 2 mm cut removes the dense skin entirely and reaches the gas porosity zone, and it doubles or triples the roughing time. Two millimeters belongs to sand or gravity castings, where variation genuinely runs that wide. It also belongs to machining practice built around a sawn or flame-cut blank rather than a die.
Does the alloy change the allowance?
Only slightly. ADC12 and A380 shrink in a similar range, so the allowance does not move much between them. What changes is machinability: silicon content wears tools faster, so the same cut takes longer in a high-silicon alloy and tool cost per part rises.
Can I machine a casting with almost no stock?
On a very stable face, 0.3 mm is workable if the die is new and the fixture is rigid. It leaves no margin for die wear, so the allowance has to be reviewed as the tool ages. Below 0.3 mm the process depends on the die staying perfect, which no production die does.
Who pays when a machined face does not clean up?
Whoever owns the drawing error. If the allowance was specified and the casting met its tolerance, the extra cut is a legitimate cost. If the allowance was never specified, the supplier carried the risk and will price it in. Settling this before the first order is cheaper than settling it after.
Should I leave stock on a face that will only be painted?
No. A painted surface hides as-cast texture, so 0.2 mm of blast and pretreatment is enough and no machining is needed. Adding stock there costs a full machining operation and opens porosity under a coating that will not seal it.
Author: HKX Engineering Team
HKX — Ningbo Hexin Mould Co., Ltd., an aluminum die casting manufacturer in Ningbo, China, with 30+ years of tooling experience, in-house machining and finishing, ISO 9001 and IATF 16949 certification, and customers in more than 20 countries.
Talk to the HKX Engineering Team
Send a drawing or a STEP model with the machined surfaces marked, and HKX will return an allowance schedule face by face, with the as-cast band, the fixture plan and the machining sequence that follows. The package includes DFM feedback on datum placement, a stock map showing available material at every machined face, sample castings for trial cuts, and first article and material reports for your quality file. Where a face cannot clean up at the agreed stock, HKX says so before the die is cut. To start the review, contact our engineering team with the model and the annual volume. The manufacturing process overview shows how casting and machining are sequenced in-house. The aluminum oil pump housing page shows a part where bore stock and sealing faces drive the whole tolerance plan.